What ASTM A320 actually covers
ASTM A320 is the specification for alloy-steel and stainless-steel bolting intended for low-temperature service. Where A193 covers high-temperature and high-pressure bolting, A320 covers the other end of the curve: flanges, valves and pipe joints that operate at cryogenic or sub-zero temperatures — LNG terminals, air separation plants, refrigeration, cold-storage piping, and winter-exposed refinery service.
The specification matters to buyers for one practical reason: at low temperature, steel loses impact toughness before it loses tensile strength. A bolt that passes a room-temperature tensile test can shatter on a cold start-up. A320 exists to force the impact test that catches this.
If you are sourcing low temperature bolts to ASTM A320, this guide covers the grades, the test that actually separates a compliant lot from a rejected one, and what to check on the mill certificate before the containers leave.
The grades you will actually be asked to quote
| Grade | Material family | Typical application | Service temperature floor |
|---|---|---|---|
| L7 | Alloy steel (AISI 4140 / 4142, quenched & tempered) | General low-temperature bolting, valves, flanges | −101 °C (−150 °F) |
| L7M | Alloy steel, modified chemistry (higher Mo, tighter limits) | Same as L7 where the spec calls for the M variant | −101 °C (−150 °F) |
| L43 | Alloy steel (4340 modified) | Heavy section bolting requiring deeper hardenability | −101 °C (−150 °F) |
| B8 | 304 stainless (AISI 304 / S30400), carbide solution treated | Cryogenic and corrosive low-temp service | −196 °C (−320 °F) |
| B8M | 316 stainless (AISI 316 / S31600) | Low temp plus chlorides / marine-adjacent | −196 °C (−320 °F) |
| B8M3 | 316L stainless (low carbon) | Welded assemblies, resistance to sensitisation | −196 °C (−320 °F) |
Two practical notes. First, L7 and L7M are the workhorses in oil & gas — most stud bolt enquiries that land with “A320” in the subject line are L7. Second, B8/B8M at cryogenic temperatures require carbide solution treatment; if the certificate does not state it, the material is not A320-compliant even if the chemistry matches 304/316.
The one test that separates A320 from A193
This is the single most misunderstood point in fastener procurement, and it causes more rejected shipments than any other issue:
- A193 B7 and A320 L7 use the same base material (AISI 4140/4142, quenched and tempered).
- The difference is the Charpy V-notch impact test at low temperature. A320 requires impact testing at the temperature specified by the purchaser (commonly −101 °C / −150 °F); A193 B7 requires no impact test at all.
- Minimum absorbed energy for L7 per ASTM A320: 27 J (20 ft-lbf) average, with no single specimen below 20 J, tested at the specified temperature.
So when a buyer writes “A320 L7” and the supplier ships “A193 B7 with an A320-style certificate”, the bolts are identical in chemistry and strength — but they are not certified to A320, because nobody hammered a notched specimen at −101 °C. On a cryogenic flange this is the difference between a compliant joint and a brittle fracture path.
This is exactly the kind of trap that a 3.1 mill test certificate review is designed to catch — see the section on MTC checks below.
Mechanical requirements at a glance
| Property | L7 / L7M | B8 | B8M |
|---|---|---|---|
| Tensile strength (min) | 860 MPa (125 ksi) | 515 MPa (75 ksi) | 515 MPa (75 ksi) |
| Yield strength (min, 0.2%) | 725 MPa (105 ksi) | 205 MPa (30 ksi) | 205 MPa (30 ksi) |
| Elongation (min, 4D) | 16% | 30% | 30% |
| Reduction of area (min) | 50% | 50% | 50% |
| Hardness | ≤ 235 HBW / ≤ 35 HRC | ≤ 96 HRB | ≤ 96 HRB |
| Impact test | Required at purchaser-specified temp | Required at purchaser-specified temp | Required at purchaser-specified temp |
| Surface finish | — | Carbide solution treated | Carbide solution treated |
Values above are the common minimums; always confirm against the edition of A320 called out in the purchase order, because supplementary requirements (S1, S2, S3…) can tighten them further.
Nuts and washers: A194 is not optional
A320 bolts are matched with ASTM A194 nuts and, where specified, ASTM F436 hardened washers. The grade pairing matters:
| Bolt grade | Matching nut grade (A194) | Common mistake |
|---|---|---|
| L7 / L7M | Gr. 4 or Gr. 7 | Shipping A194 2H (that is the A193 B7 pairing) — wrong for low-temp service |
| B8 | Gr. 8 | Using 304 nuts of unknown heat treatment |
| B8M / B8M3 | Gr. 8M | Mixing 316 bolts with 304 nuts |
The nut must also carry its own impact test where the specification requires it. A shipment that pairs A320 L7 studs with 2H nuts will be rejected at the joint level even though every individual piece passes its own tensile test — because the nut becomes the brittle link. For the nut side of the standard family, see our A563 and A194 nut grades guide.
Where A320 bolting is specified
- LNG and cryogenic terminals: B8/B8M or L7 stud bolts on cryogenic flanges, loading arms, vaporiser piping
- Air separation and industrial gas plants: cold box bolting, typically B8M
- Refineries and petrochemical: low-temperature sections, winterised units in Kazakhstan, Russia and northern China
- Gas transmission: compressor station and pipeline flanges in cold climates — the exact application behind most Central Asian enquiries we see
- Cold storage and refrigeration: ammonia plant flanges
What to verify on the mill certificate
A compliant A320 package should show, per heat number:
- Charpy impact results at the specified temperature, with individual specimen values (not just an average)
- Test temperature stated explicitly — if it says “room temperature”, the lot is not A320
- Hardness readings within the L7 ceiling (235 HBW / 35 HRC); over-hardened L7 fails toughness even if impact values pass
- Carbide solution treatment noted for B8/B8M
- Grade and standard edition clearly printed (A320 / A320M, with year)
- Heat traceability from the certificate to the head marking on the bolts
Our guide to reading a fastener MTC walks through the seven fields buyers should check on every certificate.
If your project requires witnessed testing or a 3.2 certificate, the tender and project supply documentation route is the one to discuss before the order — witnessed Charpy testing adds lead time that cannot be recovered later.
Frequently asked questions
Is A320 L7 the same as A193 B7?
Same base material and the same tensile and yield minimums, but not the same specification: A320 L7 requires Charpy V-notch impact testing at a purchaser-specified low temperature, while A193 B7 does not. Never substitute one certificate for the other.
What is the minimum impact energy for A320 L7?
27 J (20 ft-lbf) average for the specimen set, with no individual specimen below 20 J, tested at the temperature stated on the purchase order.
Can I use 304 (B8) bolts at −196 °C?
Yes, B8 and B8M are qualified for cryogenic service down to −196 °C, provided they are carbide solution treated and impact tested. Confirm the certificate states the treatment and the test temperature.
Which nuts go with A320 L7 stud bolts?
ASTM A194 Grade 4 or Grade 7. A194 2H is the correct pairing for A193 B7 at elevated temperature, not for low-temperature L7 service.
Does zinc plating affect A320 compliance?
The plating itself does not change the grade, but hydrogen can be absorbed during electroplating and cause delayed brittle failure in high-strength L7. Where plating is required on L7, specify post-plate baking and confirm the process in the inspection documents.